Case-hardening steels have low carbon (limited to about 0.25%). The surface is carburised and hardened to 57–63 HRC while the core stays tough, combining a wear-resistant surface with an impact-resistant core in the same part.

  • 4120
  • 8620≈ 20NiCrMo2-2 · 1.6523
  • 16MnCr5

Table values are the limits of the relevant standard (min–max) and do not replace the batch certificate. Mill certificates are supplied with the goods on request.

Equivalent grades

8620
≈ 20NiCrMo2-2 (1.6523) · DIN 21NiCrMo2 · AFNOR 20NCD2 · BS 805M20 (approximate equivalent)
16MnCr5
Similar group to SAE 5115

Chemical composition (%)

GradeStandardCSiMnP maxS maxCrMoNi
16MnCr5EN 100840.14–0.19max 0.401.00–1.300.0250.0350.80–1.10––
20NiCrMo2-2 (≈8620)EN0.17–0.230.15–0.400.65–0.950.0250.0350.35–0.700.15–0.250.40–0.70
8620SAE0.18–0.230.15–0.350.70–0.900.0350.0400.40–0.600.15–0.250.40–0.70
Cu max 0.40% in 20NiCrMo2-2. Composition of grade 4120 is stated on the mill certificate supplied with the goods.

Mechanical properties

20NiCrMo2-2 core properties after carburising and hardening (longitudinal)

Diameter (mm)Rm (N/mm²)Rp0.2 min (N/mm²)A min (%)KCU min (J)HB
111180–1570930727.5354–438
30830–11305901030249–339
63690–9804901130210–295

Heat treatment

20NiCrMo2-2 (°C)

Carburising
880–980
Core hardening
860–900
Case hardening after carburising
800–830
Stress relieving
150–200

Case depth (to 50 HRC)

Carburising timeDepth (mm)
1 hour0.25
4 hours0.50
8 hours0.65
Surface hardness: 64 HRC at 0.25 mm depth, 59 HRC at 0.60 mm.

Applications

16MnCr5
Piston pins, camshafts, gears (high core strength)
8620
Gears, universal joint crosses, bearing cages
4120
Piston pins, crankshafts, gears, flywheel parts