Quenched and Tempered Steels

The European equivalent of 4140 is 42CrMo4 (1.7225) and of 5140 is 41Cr4 (1.7035). Both are quenched and tempered steels under EN ISO 683-2, gaining high strength and toughness through hardening and tempering.
- 414042CrMo4 · 1.7225
- 514041Cr4 · 1.7035
Table values are the limits of the relevant standard (min–max) and do not replace the batch certificate. Mill certificates are supplied with the goods on request.
Equivalent grades
| SAE / AISI | EN | Material no. | AFNOR | BS |
|---|---|---|---|---|
| 4140 | 42CrMo4 | 1.7225 | 42CD4 | 708M40 |
| 5140 | 41Cr4 | 1.7035 | 42C4 | 530M40 |
Chemical composition (%)
| Grade | Standard | C | Si | Mn | P max | S max | Cr | Mo |
|---|---|---|---|---|---|---|---|---|
| 42CrMo4 (≈4140) | EN ISO 683-2 | 0.38–0.45 | 0.10–0.40 | 0.60–0.90 | 0.025 | 0.035 | 0.90–1.20 | 0.15–0.30 |
| 4140 | SAE | 0.38–0.43 | 0.15–0.35 | 0.75–1.00 | 0.035 | 0.040 | 0.80–1.10 | 0.15–0.25 |
| 41Cr4 (≈5140) | EN ISO 683-2 | 0.38–0.45 | 0.10–0.40 | 0.60–0.90 | 0.025 | 0.035 | 0.90–1.20 | – |
| 5140 | SAE | 0.38–0.43 | 0.15–0.35 | 0.70–0.90 | 0.035 | 0.040 | 0.70–0.90 | – |
Mechanical properties
Quenched and tempered (longitudinal, room temperature)
Standard: EN ISO 683-2| Grade | Diameter (mm) | Rm (N/mm²) | Rp0.2 min (N/mm²) | A min (%) | Z min (%) | KV min (J) | HBW |
|---|---|---|---|---|---|---|---|
| 42CrMo4 | ≤16 | 1100–1300 | 900 | 10 | 40 | – | 331–380 |
| 42CrMo4 | 16–40 | 1000–1200 | 750 | 11 | 45 | 35 | 298–359 |
| 42CrMo4 | 40–100 | 900–1100 | 650 | 12 | 50 | 35 | 271–331 |
| 42CrMo4 | 100–160 | 800–950 | 550 | 13 | 50 | 35 | 240–286 |
| 42CrMo4 | 160–250 | 750–900 | 500 | 14 | 55 | 35 | 225–271 |
| 41Cr4 | ≤16 | 1000–1200 | 800 | 11 | 30 | – | 298–359 |
| 41Cr4 | 16–40 | 900–1100 | 660 | 12 | 35 | 35 | 271–331 |
| 41Cr4 | 40–100 | 800–950 | 560 | 14 | 40 | 35 | 240–286 |
Heat treatment
Temperatures (°C)
| Process | 42CrMo4 | 41Cr4 |
|---|---|---|
| Normalising | 870, air cooling | 860, air cooling |
| Hardening | 860 oil or polymer; 820 water | 820–860 oil, polymer or water |
| Tempering | 540–680, air cooling | 540–680, air cooling |
| Soft annealing | 720, cool at 15 °C/h to 600 °C, then air | 720–740, furnace cooling |
| Critical points | AC1 745 · AC3 790 · Ms 335 | AC1 750 · AC3 790 · Ms 310 |
Applications
- 42CrMo4 is suitable for ISO 898-1 property class 10.9 fasteners (Ø ≥16 mm: Rm ≥830 N/mm², Rp0.2 ≥660 N/mm², A ≥12%, 250–316 HB).
Other product groups
Case-Hardening Steels4120 · 8620 · 16MnCr5
Carbon Engineering Steels1020 – 1080
Transmission Shafting1010 – 1020
Black Welded PipeS195T · EN 10255
Hollow SectionsS235JRH · S355J2H
Cold-Drawn Steel TubeE235 · E355 · EN 10305-1
NPI I-BeamsIPN 80 – 300
NPU ChannelsUPN 50 – 300
Equal-Leg AnglesL · EN 10056 · S235JR
Steel Sheet and PlateGuillotine and laser cut
Hot-Rolled Flat and Square BarEN 10058 · EN 10059 · S235JR
Cold-Drawn Flat and Square BarEN 10278 · h11
Cold-Drawn, Peeled and Ground Bars+C · +SH · +SL · h6–h11
Hexagon Barsby width across flats
Free-Cutting SteelC35 · C45Pb
Bearing Steel100Cr6
Spring Steel9260 · 9262 · …