Iron–carbon alloys

Steel and cast iron are alloys of iron and carbon. Because even very small amounts of carbon change hardness and strength noticeably, iron–carbon alloys are first classified by carbon content.

ClassCarbon content (approx.)General properties
SteelUp to 2% (most engineering steels below 1.1%)Can be rolled and forged; properties can be changed by heat treatment
Cast iron2 – 4.5%Shaped by casting; hard and brittle, cannot be forged

Steels by carbon content

GroupCarbonPropertiesTypical usesExample grades
Low carbon≈ up to 0.25%Soft, easy to form, good weldabilitySections, sheet, tube; case-hardened parts1010, 1020, S235JR, 16MnCr5
Medium carbon≈ 0.25 – 0.60%Balanced strength and toughness; can be hardened by quenchingShafts, axles, gears, bolts, machine parts1040, 1045 (C45), 4140
High carbon≈ above 0.60%Hard and wear resistant; lower ductilitySprings, cutting tools, bearings1070, 1080, 9260, 100Cr6
Group limits vary slightly between sources; the table gives a general framework.

How is steel made?

Steel is made in two main ways: by burning off the excess carbon in blast-furnace pig iron with oxygen, or by melting scrap steel in an electric arc furnace. Before casting, the oxygen in the steel is removed with aluminium or silicon; steel made this way is called killed steel. Almost all engineering steels are killed, then take their final form by hot rolling, forging or cold drawing.

Carbon steel and alloy steel

In carbon (non-alloy) steel, elements other than carbon stay below certain limits. A widely used definition sets these at 1.65% manganese, 0.60% silicon and 0.60% copper. Steels that exceed these limits, or to which elements such as chromium, nickel or molybdenum are deliberately added, are called alloy steels.

  • Low-alloy steels: total alloying content usually below 5%. Quenched and tempered steels (4140, 5140), case-hardening steels (8620, 16MnCr5) and bearing steel (100Cr6) belong here.
  • High-alloy steels: total alloying content above 5%, such as stainless and tool steels.

The main advantage of alloy steels is hardenability: they harden through to the core even in thick sections and, after heat treatment, combine high strength with toughness. A shaft of the same size hardens only at the surface in carbon steel, while alloy steel gives a much more even hardness across the section.

Effect of alloying elements

The elements you see in chemical composition tables affect the steel as follows:

Carbon (C)
The element that raises hardness and strength the most. More carbon means better hardening response and wear resistance, but lower ductility, toughness and weldability.
Manganese (Mn)
Raises strength and hardenability. Binds sulphur and so prevents cracking during hot working.
Silicon (Si)
Used to remove oxygen during steelmaking. Raises strength and elasticity; present in high amounts in spring steels (9260, 9262).
Phosphorus (P)
Usually an unwanted impurity. Kept to a low maximum in standards because it causes brittleness, especially at low temperatures.
Sulphur (S)
Unwanted in most steels as it causes hot shortness. Deliberately added to free-cutting steels so that chips break short.
Chromium (Cr)
Raises hardenability, wear resistance and strength. Above 12% it makes steel stainless. 4140, 5140 and 100Cr6 are chromium steels.
Nickel (Ni)
Raises toughness, especially impact strength at low temperature, and contributes to hardenability. Present in 8620.
Molybdenum (Mo)
Raises hardenability, reduces temper embrittlement and retains strength at high temperature. Present in 4140 and 8620.
Vanadium (V)
Refines the grain structure; raises toughness and wear resistance.
Tungsten (W)
Helps keep hardness at high temperature; a key element of high-speed steels.
Aluminium (Al)
Used as a deoxidiser and grain refiner; forms a hard surface layer in nitriding steels.
Copper (Cu)
Improves resistance to atmospheric corrosion; in high amounts it can cause surface cracking during hot working.
Lead (Pb)
Improves machinability; found in leaded free-cutting steels (C45Pb, 11SMnPb30).

Heat treatment

Heat treatment means heating steel to a set temperature, holding it there and cooling it in a controlled way to change its internal structure and so its mechanical properties. The same grade can give very different hardness and strength depending on the treatment applied.

Softening and conditioning

Normalising
The steel is heated above its transformation temperature and cooled in air. The grain becomes finer and more uniform, correcting the structure after rolling or forging.
Soft annealing
The steel is heated and cooled very slowly in the furnace. Hardness drops, making machining and cold forming easier.
Spheroidising
In high-carbon steels the carbides are brought into a spherical shape, giving the softest and most machinable condition. Bearing steel is usually supplied in this condition (+AC).
Stress relieving
Done at a lower temperature to reduce internal stresses left by welding, machining or cold forming; structure and hardness do not change noticeably.

Hardening processes

Quenching
The steel is heated above its transformation temperature and cooled rapidly in water, oil or polymer solution. A very hard but brittle structure called martensite forms. Steels with less than about 0.25% carbon do not harden noticeably on quenching.
Tempering
Quenched steel is reheated to a lower temperature. Some hardness is traded for toughness and brittleness is removed. Quenching followed by tempering is called quenching and tempering (+QT).
Case hardening (carburising)
Carbon is diffused into the surface of low-carbon steel at high temperature, followed by quenching. The surface becomes hard and wear resistant (about 57–63 HRC) while the core stays tough. Used for gears, pins and camshafts.
Induction hardening
Only the surface of a medium-carbon steel (e.g. C45) is heated rapidly by electric induction and quenched. Used where local hardness is needed, such as bearing seats and gear flanks.

Heat-treatment temperatures and times depend on the grade. Grade-specific values are given in the heat-treatment tables on the product pages.

Delivery condition and tolerance codes

The codes on product pages and certificates show the condition in which the material is supplied:

CodeMeaning
+ARAs rolled, not heat treated
+NNormalised
+ASoft annealed
+ACAnnealed to spheroidised carbides
+QTQuenched and tempered
+CCold drawn
+SHPeeled
+SLGround

Codes such as h6, h9 and h11 are shaft tolerance classes to ISO 286. The letter "h" means the size never exceeds the nominal value and may only deviate downwards. The smaller the number, the tighter the tolerance: h6 is typical of ground bars, h9–h11 of cold-drawn and peeled bars.

Glossary

Austenite
The crystal structure of steel at high temperature. For quenching and normalising, steel is first heated into this structure.
Corrosion
Deterioration of a metal through chemical or electrochemical reaction with its surroundings. Rusting is its best-known form in steel.
Dislocation
A line defect in the crystal lattice. Metals deform permanently by the movement of dislocations; cold working increases their number and so hardens the material.
Ductility
The ability of a material to deform permanently before breaking, expressed as elongation (A) and reduction of area (Z).
Elongation (A)
The permanent increase in length of a broken tensile specimen as a percentage of its original length.
Enamel
A glass-based protective and decorative coating fused onto a metal surface at high temperature.
Ferrite
The soft, ductile crystal structure of iron at room temperature; it can dissolve very little carbon.
Galvanising
Coating steel with zinc to protect it from corrosion. Hot-dip galvanising is the most common method.
Hardenability
How deep steel hardens when quenched. High in alloy steels, so the core of thick parts hardens too.
Hardness
Resistance of a surface to a hard indenter pressed into it. Measured by the Brinell (HB), Rockwell (HRC) and Vickers (HV) methods.
Machinability
How easily, cleanly and with how little tool wear a material can be turned or milled. Raised in free-cutting steels by sulphur and lead.
Martensite
The very hard, brittle structure formed by quenching, in which carbon is trapped in the iron lattice. Its toughness is raised by tempering.
Modulus of elasticity
The stiffness of a material in the elastic range: the ratio of stress to strain. About 210 GPa for steel and almost independent of grade.
Pearlite
A structure of alternating ferrite and cementite (iron carbide) layers, found in slowly cooled carbon steels.
Reduction of area (Z)
The percentage decrease in cross-section at the fracture of a tensile specimen; a measure of ductility.
Solid solution
A single-phase structure in which atoms of one element are dissolved in the crystal lattice of another metal, such as carbon dissolved in iron.
Strength
The general term for a material’s ability to carry load without breaking or deforming permanently.
Tensile strength (Rm)
The highest stress a material carries before breaking in a tensile test, given in MPa (N/mm²).
Toughness
The ability of a material to absorb energy before fracture, measured by notched impact tests (KV, KU, joules). A hard material that is not tough breaks under sudden load.
Weldability
How well steel can be welded without cracking or losing its properties. Falls as carbon and alloy content rise; assessed with the carbon equivalent (CEV).
Yield strength (Re, Rp0.2)
The stress at which a material starts to deform permanently. For steels without a distinct yield point, the stress at 0.2% permanent strain (Rp0.2) is used.